1. General considerations
The quality of PE pipe welding is dependent on:
2. Pre-welding tips
The welding area should be protected from inappropriate atmospheric factors such as moisture or temperatures below +5 ̊C. If one side is warmer than another side due to intense sunlight, non-uniform heat generation on pipe surface should be prevented using an umbrella or tent. Wind and air currents also should be prevented during welding by closing the pipe ends.
PE pipes that are transported as coils have an oval cross section immediately after opening. Accordingly, the welding area should be first turned into a circle using hot air or a mold before welding. The welding area should be free of any dust and oil. So the welding area should be carefully cleaned before welding.
3. Butt fusion
Any welding machine has its own specifications regarding welding force or pressure as often reported by manufacturers. To obtain the force or pressure required for welding, the welding pressure should be calculated from welding area and added to the machine force read from pressure gage. In other words, the total welding pressure equals the pressure for moving the machine plus the pressure required for welding per unit area. After cutting and flattening the welding area, the fillings should be removed by a brush. Do not touch the welded section. The both welding surfaces should be cleaned before welding by ethanol 99% using a soft paper.
After joining the pipes, the gap between them and level are controlled. The gap between the two pipes should be in accordance with relevant standards (Table 1).
The difference between the areas of two pipes can be up to 10% of the pipe thickness, but not more than 0.5 mm.
4. Fastening
In this case, the two pipes are pressed to the hot plate from both sides uniformly. An edge is formed on both sides of the plate. Fastening is completed when an edge with specifications in the second row of Table 2 is formed.
5. Heating
Upon formation of the welding edge, pressure is reduced to a minimum of 0.02 N/mm2 and heating is started. Heat diffuses the welding area to prepare the thermoplastic pipe for welding. Heating duration can be found in the third raw of Table 2.
6. Conversion
Upon completion of heating, the plate should be slowly removed to avoid damage to the welding area and then the two pipes should be immediately connected. The two pipes are slowly connected to each other. Conversion should take a short time, otherwise it will damage welding quality. Conversion time is noted in the fourth row of Table 2.
7. Welding
Two pipe surfaces approach each other with an approximate speed of 0. The pressure is then increased to a maximum permissible limit after an interval specified in the fifth row of Table 2. The pressure required for welding is 0.015 N/mm2.
8. Cooling
A constant welding pressure is maintained during cooling (fifth row of Table 2). After completion of all butt fusion stages, the shape in Fig. 3 should be formed at welding site. Figure 4 shows welding stages on the diagram.
Hydraulic tests (internal pressure test) should be performed prior to operation to ensure sealing of...
Installation of pipes is started after delivery of pipes, fittings and other necessary tools. Pipes ...